| SAE 1010 | ||||
| Chemical composition: C=0.10%, Mn=0.45%, P=0.04% max, S=0.05% max | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 200 | GPa | 29000 | ksi | 
| Thermal expansion (20 ºC) | 12.6*10-6 | ºCˉ¹ | 7.00*10-6 | in/(in* ºF) | 
| Specific heat capacity | 448 | J/(kg*K) | 0.107 | BTU/(lb*ºF) | 
| Thermal conductivity | 51.9 | W/(m*K) | 360 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 1.43*10-7 | Ohm*m | 1.43*10-5 | Ohm*cm | 
| Tensile strength (hot rolled) | 325 | MPa | 47100 | psi | 
| Yield strength (hot rolled) | 180 | MPa | 26100 | psi | 
| Elongation (hot rolled) | 28 | % | 28 | % | 
| Hardness (hot rolled) | 55 | RB | 55 | RB | 
| Tensile strength (cold drawn) | 365 | MPa | 52900 | psi | 
| Yield strength (cold drawn) | 305 | MPa | 44200 | psi | 
| Elongation (cold drawn) | 20 | % | 20 | % | 
| Hardness (cold drawn) | 60 | RB | 60 | RB | 