| SAE 1030 | ||||
| Chemical composition: C=0.30%, Mn=0.75%, P=0.04% max, S=0.05% max | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.872 *10³ | kg/m³ | 491.4 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 200 | GPa | 29000 | ksi | 
| Thermal expansion (20 ºC) | 11.7*10-6 | ºCˉ¹ | 6.5*10-6 | in/(in* ºF) | 
| Specific heat capacity | 486 | J/(kg*K) | 0.116 | BTU/(lb*ºF) | 
| Thermal conductivity | 48.7 | W/(m*K) | 338 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 1.66*10-7 | Ohm*m | 1.66*10-5 | Ohm*cm | 
| Tensile strength (hot rolled) | 470 | MPa | 68200 | psi | 
| Yield strength (hot rolled) | 260 | MPa | 37700 | psi | 
| Elongation (hot rolled) | 20 | % | 20 | % | 
| Hardness (hot rolled) | 75 | RB | 75 | RB | 
| Tensile strength (cold drawn) | 525 | MPa | 76100 | psi | 
| Yield strength (cold drawn) | 440 | MPa | 63800 | psi | 
| Elongation (cold drawn) | 12 | % | 12 | % | 
| Hardness (cold drawn) | 80 | RB | 80 | RB | 