Main page
 About us
 Sliding Bearings Consulting
 Advertising Opportunities


to Metals
 to Aluminum alloys
The following casting methods are applicable for casting aluminum alloys:
Sand casting, permanent mold casting, die casting, investment casting, centrifugal casting, squeeze casting and continuous casting.
 
 to top
Classification of cast aluminum alloys is developed by the Aluminum Association of the United States:
Each cast alloy is designated by a four digit number with a decimal point separating the third and the forth digits.
1xx.x aluminum, 99.0% minimum;
2xx.x copper (4%...4.6%);
3xx.x silicon (5%...17%) with added copper and/or magnesium;
4xx.x silicon (5%...12%);
5xx.x magnesium (4%...10%);
7xx.x zinc (6.2%...7.5%);
8xx.x tin;
9xx.x others.
In the alloys of the 1xx.x series the second two digits indicate the level of purity of the alloy – they are the same as the two digits to the right of the decimal point in the minimum concentration of aluminum (in percents): 150.0 means minimum 99.50% of aluminum in the alloy, 120.1 means minimum 99.20% of aluminum in the alloy.
In all other groups of aluminum alloys (2xx.x through 9xx.x) the second two digits signify different alloys in the group.
 A modification of the original alloy or impurity limits is indicated by a serial letter before the numerical designation. The serial letters are assigned in alphabetical order starting with A but omitting I, O, Q, and X (the letter “X” is reserved for experimental alloys).
 
 to top
Aluminum-copper cast alloys (2xx.x series)
Applications:
Cylinder heads for automotive and aircraft engines, pistons for diesel engines, exhausting system parts.
Aluminum-silicon-copper/magnesium cast alloys (3xx.x series)
Applications:
Automotive cylinder blocks and head, car wheels, aircraft fittings, casings and other parts of compressors and pumps.
Aluminum-silicon cast alloys (4xx.x series)
Applications:
Pump casings, thin wall castings, cookware.
Aluminum- magnesium cast alloys (5xx.x series)
Applications:
Sand cast parts.
Aluminum-zinc cast alloys (7xx.x series)
Aluminum-tin cast alloys (8xx.x series)
Applications:
Monometal (solid) and bi-metal slide bearings for internal combustion engines and other slide bearings applications.
 
 to top
| Designation | Si,% | Cu,% | Mn,% | Mg,% | Zn,% | Ti,% | Others,% | 
|---|---|---|---|---|---|---|---|
| 201.0 | 0.1 max. | 4.0-5.2 | 0.2-0.5 | 0.15-0.55 | - | 0.15-0.35 | Ag 0.4-1.0 | 
| 208.0 | 2.5-3.5 | 3.5-4.5 | 0.5 max. | 0.1 max. | 1.0 max. | 0.25 max. | - | 
| 222.0 | 2.0 max. | 9.2-10.7 | 0.5 max. | 0.15-0.35 | 0.8 max. | 0.25 max. | - | 
| 333.0 | 8.0-10.0 | 3.0-4.0 | 0.5 max. | 0.05-0.5 | 1.0 max. | 0.25 max. | - | 
| 356.0 | 6.5-7.5 | 0.25 max. | 0.35 max. | 0.2-0.45 | 0.35 max. | 0.25 max. | - | 
| 413.0 | 11.0-13.0 | 1.0 max. | 0.35 max. | 0.1 max. | 0.5 max. | - | - | 
| 443.0 | 4.5-6.0 | 0.6 max. | 0.5 max. | 0.05 max. | 0.5 max. | 0.25 max. | - | 
| 514.0 | 0.35 max. | 0.15 max. | 0.35 max. | 3.5-4.5 | 0.15 max. | 0.25 max. | - | 
| 518.0 | 0.35 max. | 0.25 max. | 0.35 max. | 7.5-8.5 | 0.15 max. | - | - | 
| 705.0 | 0.2 max. | 0.20 max. | 0.4-0.6 | 1.4-1.8 | 2.7-3.3 | 0.25 max. | Cr 0.2-0.4 | 
| 713.0 | 0.25 max. | 0.4-1.0 | 0.6 max. | 0.2-0.5 | 7.0-8.0 | 0.25 max. | - | 
| 852.0 | 0.4 max. | 1.7-2.3 | 0.1 max. | 0.6-0.9 | - | 0.25 max. | Sn5.5-7.0, Ni0.9-1.5 | 
(concentration of aluminum - balance)
 