| Cast copper alloy C97600 (Nickel-Silver 20% Ni) | ||||
| Chemical composition: Ni=20.3%, Zn=6.0%, Sn=4.0%, Pb=4.0% Cu=balance | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.89 *10³ | kg/m³ | 555 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 131 | GPa | 19000 | ksi | 
| Thermal expansion (20 ºC) | 16.7*10-6 | ºCˉ¹ | 9.3*10-6 | in/(in* ºF) | 
| Specific heat capacity | 377 | J/(kg*K) | 0.090 | BTU/(lb*ºF) | 
| Thermal conductivity | 22.6 | W/(m*K) | 156 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 34.5*10-8 | Ohm*m | 34.5*10-6 | Ohm*cm | 
| Tensile strength (sand cast) | 310 | MPa | 45000 | psi | 
| Yield strength (sand cast) | 165 | MPa | 24000 | psi | 
| Elongation (sand cast) | 20 | % | 20 | % | 
| Fatigue strength (sand cast) | 107 | MPa | 16000 | psi | 
| Hardness (sand cast) | 80 | HB(500) | 80 | HB(500) | 
| Liquidus temperature | 1143 | ºC | 2089 | ºF | 
| Solidus temperature | 1108 | ºC | 2027 | ºF | 