| Commercially pure nickel 200 | ||||
| Chemical composition: Ni=99% min. | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.89 *10³ | kg/m³ | 555 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 207 | GPa | 30000 | ksi | 
| Thermal expansion (20 ºC) | 13.3*10-6 | ºCˉ¹ | 7.4*10-6 | in/(in* ºF) | 
| Specific heat capacity | 456 | J/(kg*K) | 0.109 | BTU/(lb*ºF) | 
| Thermal conductivity | 70.2 | W/(m*K) | 487 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 9.5*10-8 | Ohm*m | 9.5*10-6 | Ohm*cm | 
| Tensile strength (annealed) | 462 | MPa | 67000 | psi | 
| Yield strength (annealed) | 148 | MPa | 21500 | psi | 
| Elongation (annealed) | 45 | % | 45 | % | 
| Liquidus temperature | 1446 | ºC | 2635 | ºF | 
| Solidus temperature | 1436 | ºC | 2615 | ºF |