to Metals
 Gold (Au) is a transition metal with an atomic number 79.
 The atomic mass of gold is 196.966569 (naturally occurring isotope).
 A nucleus of gold is composed of 76 protons and 118 neutrons.
 
 Gold is found in hydrothermal quartz veins mostly in chemically uncombined metallic state. The natural gold is commonly alloyed with silver with minor amounts of platinum, copper and other metals. The natural gold-silver alloy is called electrum.
 Gold occurs also in a combined form as AuTe2 (telluride of gold). The minerals containing telluride of gold are calaverite and sylvanite.
 
  The three most prominent properties of gold:
 
 Pure gold is very soft (25 HV) therefore it is rarely used in an non-alloyed state.
 The strength, modulus of elasticity and hardness of gold may be considerably increased by alloying with other metals (silver, copper, nickel, zinc, palladium, platinum, iron, aluminum).
 
 Gold alloys are classified according to their purity and color.
 Purity of gold alloys is measured in carats (karats).
 The purity in carats (caratage) CK may be calculated from the concentration in % C% by the formula:
 
 CK = 0.24*C%
 
 For example the caratage of an alloy containing 75% of gold is CK = 18K
 The caratage of gold alloys may vary between 9K to 24K (pure gold).
 
    to top
| Carat purity and color | Au,% | Ag,% | Cu,% | Pd,% | Pt,% | Ni,% | Zn,% | Fe,% | Cd,% | Al,% | 
|---|---|---|---|---|---|---|---|---|---|---|
| 24K Yellow Gold | 99.7 min. | - | - | - | - | - | - | - | - | - | 
| 22K Yellow Gold | 92 | 4 | 4 | - | - | - | - | - | - | - | 
| 22K Yellow Gold | 91.7 | 5 | 2 | - | - | - | 1.3 | - | - | - | 
| 18K Yellow Gold | 75 | 15 | 10 | - | - | - | - | - | - | - | 
| 18K Red Gold | 75 | - | 25 | - | - | - | - | - | - | - | 
| 18K Rose Gold | 75 | 2.75 | 22.25 | - | - | - | - | - | - | - | 
| 18K Pink Gold | 75 | 5 | 20 | - | - | - | - | - | - | - | 
| 18K White Gold | 75 | - | - | 25 | - | - | - | - | - | - | 
| 18K White Gold | 75 | - | - | - | 25 | - | - | - | - | - | 
| 70Gold-30Pt | 75 | - | - | - | 30 | - | - | - | - | - | 
| 18K White Gold | 75 | - | - | 10 | - | 10 | 5 | - | - | - | 
| 18K White Gold | 75 | 18.5 | 1 | - | - | - | 5.5 | - | - | - | 
| 18K Blue Gold | 75 | - | - | - | - | - | - | 25 | - | - | 
| 18K Grey-White Gold | 75 | - | 8 | - | - | - | - | 17 | - | - | 
| 18K Green Gold | 75 | 20 | 5 | - | - | - | - | - | - | - | 
| 18K Light Green Gold | 75 | - | 23 | - | - | - | - | - | 2 | - | 
| 18K Soft Green Gold | 75 | 25 | - | - | - | - | - | - | - | - | 
| 18K Deep Green Gold | 75 | 15 | 6 | - | - | - | - | - | 4 | - | 
| 18K Purple Gold | 80 | - | - | - | - | - | - | - | - | 20 | 
| 14K Yellow Gold | 58 | 4-28 | 14-28 | - | - | - | - | - | - | - | 
| 14K White Gold | 59 | - | 25.5 | - | - | 12.3 | 3.2 | - | - | - | 
| 14K Green Gold | 58.3 | 32.5 | 9 | - | - | - | 0.2 | - | - | - | 
| 9K Yellow Gold | 37.5 | 12.1 | 44.4 | - | - | - | 6 | - | - | - | 
| 9K White Gold | 37.5 | - | 34 | - | - | 17.7 | 10.8 | - | - | - |