| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RE 100 1/8” | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Knoop | 
|---|---|---|---|---|---|---|---|---|---|---|
| 55.5 | 90 | 9 | - | 90 | 76 | 62.5 | 157 | 185 | 192 | 201 | 
| 55 | 89 | 8 | - | 89.5 | 75.5 | 61.5 | 154 | 180 | 188 | 196 | 
| 54 | 88 | 7 | - | 89.3 | 75 | 60.5 | 151 | 176 | 184 | 192 | 
| 53.5 | 87 | 6 | - | 89 | 74.5 | 59.5 | 148 | 172 | 180 | 188 | 
| 53 | 86 | 5 | - | 88.5 | 74 | 58.5 | 145 | 169 | 176 | 184 | 
| 52.5 | 85 | 4 | - | 88.3 | 73.5 | 58 | 142 | 165 | 172 | 180 | 
| 52 | 84 | 3 | - | 88 | 73 | 57 | 140 | 162 | 168 | 176 | 
| 51 | 83 | 2 | - | 87.5 | 72 | 56 | 137 | 159 | 164 | 173 | 
| 50.5 | 82 | 1 | - | 87.3 | 71.5 | 55 | 135 | 156 | 160 | 170 | 
| 50 | 81 | - | - | 87 | 71 | 54 | 133 | 153 | 156 | 167 | 
| 49.5 | 80 | - | - | 86.5 | 70 | 53 | 130 | 150 | 152 | 164 | 
| 49 | 79 | - | - | 86.3 | 69.5 | 52 | 128 | 147 | 148 | 161 | 
| 48.5 | 78 | - | - | 86 | 68 | 51 | 126 | 144 | 144 | 158 | 
| 48 | 77 | - | - | 85.5 | 68 | 50 | 124 | 141 | 141 | 155 | 
| 47 | 76 | - | - | 85.3 | 67.5 | 49 | 122 | 139 | 139 | 152 | 
| 46.5 | 75 | - | - | 85 | 67 | 48.5 | 120 | 137 | 137 | 150 | 
| 46 | 74 | - | - | 84.8 | 66 | 47.5 | 118 | 135 | 135 | 147 | 
| 45.5 | 73 | - | - | 84.5 | 65.5 | 46.5 | 116 | 132 | 132 | 145 | 
| 45 | 72 | - | - | 84 | 65 | 45.5 | 114 | 130 | 130 | 143 | 
| 44.5 | 71 | - | 100 | 83.8 | 64 | 44.5 | 112 | 127 | 127 | 141 | 
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RE 100 1/8” | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Knoop | 
| 44 | 70 | - | 99.5 | 83.5 | 63.5 | 43.5 | 110 | 125 | 125 | 139 | 
| 43.5 | 69 | - | 99 | 83 | 62.5 | 42.5 | 109 | 123 | 123 | 137 | 
| 43 | 68 | - | 98 | 82.8 | 62 | 41.5 | 107 | 121 | 120 | 135 | 
| 42.5 | 67 | - | 97.5 | 82.5 | 61.5 | 40.5 | 106 | 119 | 118 | 133 | 
| 42 | 66 | - | 97 | 82 | 60.5 | 39.5 | 104 | 117 | 116 | 131 | 
| 41.8 | 65 | - | 96 | 81.8 | 60 | 38.5 | 102 | 116 | 115 | 129 | 
| 41.5 | 64 | - | 95.5 | 81.5 | 59.5 | 37.5 | 101 | 114 | 114 | 127 | 
| 41 | 63 | - | 95 | 81 | 58.5 | 36.5 | 99 | 112 | 113 | 126 | 
| 40.5 | 62 | - | 94.5 | 80.8 | 58 | 35.5 | 98 | 110 | 112 | 124 | 
| 40 | 61 | - | 93.5 | 80.5 | 57 | 34.5 | 96 | 108 | 111 | 122 | 
| 39.5 | 60 | - | 93 | 80.3 | 56.5 | 33.5 | 95 | 107 | 110 | 120 | 
| 39 | 59 | - | 92.5 | 80 | 56 | 32 | 94 | 106 | 108 | 118 | 
| 38.5 | 58 | - | 92 | 79.5 | 55 | 31 | 92 | 104 | 107 | 117 | 
| 38 | 57 | - | 91 | 79.3 | 54.5 | 30 | 91 | 102 | 106 | 115 | 
| 37.8 | 56 | - | 90.5 | 79 | 54 | 29 | 90 | 101 | 105 | 114 | 
| 37.5 | 55 | - | 90 | 78.5 | 53 | 28 | 89 | 99 | 104 | 112 | 
| 37 | 54 | - | 89.5 | 78.3 | 52.5 | 27 | 87 | - | 103 | 111 | 
| 36.5 | 53 | - | 89 | 78 | 51.5 | 26 | 86 | - | 102 | 110 | 
| 36 | 52 | - | 88 | 77.5 | 51 | 25 | 85 | - | 101 | 109 | 
| 35.5 | 51 | - | 87.5 | 77.3 | 50.5 | 24 | 84 | - | 100 | 108 | 
| 35 | 50 | - | 87 | 77 | 49.5 | 23 | 83 | - | 100 | 107 | 
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RE 100 1/8” | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Knoop | 
| 34.8 | 49 | - | 86.5 | 76.5 | 49 | 22 | 82 | - | 99 | 106 | 
| 34.5 | 48 | - | 85.5 | 76.3 | 48.5 | 20.5 | 81 | - | 98 | 105 | 
| 34 | 47 | - | 85 | 76 | 47.5 | 19.5 | 80 | - | 97 | 104 | 
| 33.5 | 46 | - | 84.5 | 75.5 | 47 | 18.5 | 79.5 | - | 96 | 103 | 
| 33 | 45 | - | 84 | 75.3 | 46 | 17.5 | 79 | - | 95 | 102 | 
| 32.5 | 44 | - | 83.5 | 75 | 45.5 | 16.5 | 78 | - | 95 | 101 | 
| 32 | 43 | - | 82.5 | 74.5 | 45 | 15.5 | 77 | - | 94 | 100 | 
| 31.5 | 42 | - | 82 | 74.3 | 44 | 14.5 | 76 | - | 93 | 99 | 
| 31 | 41 | - | 81.5 | 74 | 43.5 | 13.5 | 75 | - | 92 | 98 | 
| 30.8 | 40 | - | 81 | 73.5 | 43 | 12.5 | 74.5 | - | 91 | 97 | 
| 30.5 | 39 | - | 80 | 73.3 | 42 | 11 | 74 | - | 90 | 96 | 
| 30 | 38 | - | 79.5 | 73 | 41.5 | 10 | 73 | - | 90 | 95 | 
| 29.5 | 37 | - | 79 | 72.5 | 40.5 | 9 | 72 | - | 89 | 94 | 
| 29 | 36 | - | 78.5 | 72.3 | 40 | 8 | 71.5 | - | 88 | 93 | 
| 28.5 | 35 | - | 78 | 72 | 39.5 | 7 | 71 | - | 88 | - | 
| 28 | 34 | - | 77 | 71.5 | 38.5 | 6 | 70 | - | 87 | - | 
| 27.8 | 33 | - | 76.5 | 71.3 | 38 | 5 | 69 | - | 87 | - | 
| 27.5 | 32 | - | 76 | 71 | 37.5 | 4 | 68.5 | - | 86 | - | 
| 27 | 31 | - | 75.5 | 70.8 | 36.5 | 3 | 68 | - | 86 | - | 
| 26.5 | 30 | - | 75 | 70.5 | 36 | 2 | 67 | - | 85 | - | 
| 26 | 29 | - | 74 | 70 | 35.5 | 1 | 66.5 | - | 85 | - | 
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RE 100 1/8” | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Knoop | 
| 25.5 | 28 | - | 73.5 | 69.8 | 34.5 | - | 66 | - | 84 | - | 
| 25 | 27 | - | 73 | 69.5 | 34 | - | 65.5 | - | 84 | - | 
| 24.5 | 26 | - | 72.5 | 69 | 33 | - | 65 | - | 83 | - | 
| 24.3 | 25 | - | 72 | 68.8 | 32.5 | - | 64 | - | 83 | - | 
| 24 | 24 | - | 71 | 68.5 | 32 | - | 63.5 | - | 82 | - | 
| 23.5 | 23 | - | 70.5 | 68 | 31 | - | 63 | - | 82 | - | 
| 23 | 22 | - | 70 | 67.8 | 30.5 | - | 62.5 | - | 81 | - | 
| 22.5 | 21 | - | 69.5 | 67.5 | 29.5 | - | 62 | - | 81 | - | 
| 22 | 20 | - | 68.5 | 67.3 | 29 | - | 61.5 | - | 80 | - | 
| 21.5 | 19 | - | 68 | 67 | 28.5 | - | 61 | - | 80 | - | 
| 21.3 | 18 | - | 67.5 | 66.5 | 27.5 | - | 60.5 | - | 79 | - | 
| 21 | 17 | - | 67 | 66.3 | 27 | - | 60 | - | 79 | - | 
| 20.5 | 16 | - | 66.5 | 66 | 26 | - | 59.5 | - | 78 | - | 
| 20 | 15 | - | 65.5 | 65.5 | 25.5 | - | 59 | - | 78 | - | 
| - | 14 | - | 65 | 65.3 | 25 | - | 58.5 | - | 77 | - | 
| - | 13 | - | 64.5 | 65 | 24 | - | 58 | - | 77 | - | 
| - | 12 | - | 64 | 64.5 | 23.5 | - | 57.7 | - | 76 | - | 
| - | 11 | - | 63.5 | 64.3 | 23 | - | 57.3 | - | 76 | - | 
| - | 10 | - | 62.5 | 64 | 22 | - | 57 | - | 75 | - | 
| - | 9 | - | 62 | 63.8 | 21.5 | - | 56.7 | - | 75 | - | 
| - | 8 | - | 61.5 | 63.5 | 20.5 | - | 56.3 | - | 74 | - | 
| - | 7 | - | 61 | 63 | 20 | - | 56 | - | 74 | - | 
| - | 6 | - | 60.5 | 62.8 | 19.5 | - | 55.5 | - | 73 | - | 
| - | 5 | - | 60 | 62.5 | 18.5 | - | 55 | - | 73 | - | 
| - | 4 | - | 59 | 62 | 18 | - | 54.7 | - | 72 | - | 
| - | 3 | - | 58.5 | 61.8 | 17 | - | 54.3 | - | 72 | - | 
| - | 2 | - | 58 | 61.5 | 16.5 | - | 54 | - | 71 | - | 
| - | 1 | - | 57.5 | 61 | 16 | - | 53.5 | - | 71 | - | 
| - | - | - | 57 | 60.8 | 15 | - | 53 | - | 70 | - | 
| RA 60 Brale | RB 100 1/16” | RC 150 Brale | RE 100 1/8” | R15T 1/16” | R30T 1/16” | R45T 1/16” | HB 500 10mm | HB 3000 10mm | HV Diamond Pyramid | Knoop |