Heat-treatable Nickel-Chromium-Iron Alloy Inconel X-750 | ||||
Chemical composition: Cr=15.5%,Fe=7%, Al=0.7%,Ti=2.5%,Mo=9%,Nb=1%,Ni=70% min. | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.28 *10³ | kg/m³ | 517 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 214 | GPa | 31000 | ksi |
Thermal expansion (20 ºC) | 12.6*10-6 | ºCˉ¹ | 7.0*10-6 | in/(in* ºF) |
Specific heat capacity | 431 | J/(kg*K) | 0.103 | BTU/(lb*ºF) |
Thermal conductivity | 12.0 | W/(m*K) | 83.3 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 122*10-8 | Ohm*m | 122*10-6 | Ohm*cm |
Tensile strength (precip. hard) | 1250 | MPa | 181000 | psi |
Yield strength (precip. hard.) | 850 | MPa | 123000 | psi |
Elongation (precip. hardened) | 30 | % | 30 | % |
Solution temperature | 1150 | ºC | 2100 | ºF |
Aging temperature | 843 | ºC | 1550 | ºF |
Aging time | 24 | hrs. | 24 | hrs. |
Liquidus temperature | 1430 | ºC | 2610 | ºF |
Solidus temperature | 1390 | ºC | 2530 | ºF |