Nickel-Copper Alloy (Monel K-500) | ||||
Chemical composition: Cu=30%, Al=2.7%, Ti=0.6% Ni=63% min. | ||||
Property | Value in metric unit | Value in US unit | ||
Density | 8.44 *10³ | kg/m³ | 527 | lb/ft³ |
---|---|---|---|---|
Modulus of elasticity | 179 | GPa | 26000 | ksi |
Thermal expansion (20 ºC) | 13.7*10-6 | ºCˉ¹ | 7.6*10-6 | in/(in* ºF) |
Specific heat capacity | 419 | J/(kg*K) | 0.10 | BTU/(lb*ºF) |
Thermal conductivity | 17.5 | W/(m*K) | 121 | BTU*in/(hr*ft²*ºF) |
Electric resistivity | 61.5*10-8 | Ohm*m | 61.5*10-6 | Ohm*cm |
Tensile strength (precip. hard) | 1100 | MPa | 160000 | psi |
Yield strength (precip. hard.) | 630 | MPa | 91400 | psi |
Elongation (precip. hardened) | 25 | % | 25 | % |
Liquidus temperature | 1350 | ºC | 2460 | ºF |
Solidus temperature | 1300 | ºC | 2370 | ºF |