to Wrought aluminum-copper alloys (2xxx)
 to Properties of aluminum alloys 
(submitted by the website administration)
 
| Wrought aluminum alloy 2017 | ||||
| Chemical composition: Si=0.50%,Cu=4.0%, Mn=0.70%, Mg = 0.60%, Al balance | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 2.79 *10³ | kg/m³ | 174 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 72 | GPa | 10500 | ksi | 
| Thermal expansion (20 ºC) | 23.6*10-6 | ºCˉ¹ | 13.1*10-6 | in/(in* ºF) | 
| Specific heat capacity | 880 | J/(kg*K) | 0.21 | BTU/(lb*ºF) | 
| Thermal conductivity | 193 | W/(m*K) | 1340 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 3.49*10-8 | Ohm*m | 3.49*10-6 | Ohm*cm | 
| Tensile strength (annealed) | 179 | MPa | 26000 | psi | 
| Yield strength (annealed) | 69 | MPa | 10000 | psi | 
| Elongation (annealed) | 22 | % | 22 | % | 
| Shear strength (annealed) | 124 | MPa | 18000 | psi | 
| Fatigue strength (annealed) | 90 | MPa | 13000 | psi | 
| Hardness (annealed) | 45 | HB | 45 | HB | 
| Tensile strength (T651) | 427 | MPa | 62000 | psi | 
| Yield strength (T651) | 28 | MPa | 40000 | psi | 
| Elongation (T651) | 22 | % | 22 | % | 
| Shear strength (T651) | 262 | MPa | 38000 | psi | 
| Fatigue strength (T651) | 124 | MPa | 18000 | psi | 
| Hardness (T651) | 105 | HB | 105 | HB | 
| Annealing temperature | 413 | ºC | 775 | ºF | 
| Solution temperature | 505 | ºC | 940 | ºF | 
| Aging temperature | 22 | ºC | 72 | ºF |