| Non-heat-treatable Nickel-Chromium-Iron Alloy Incoloy 800 | ||||
| Chemical composition: Cr=21%, Fe=39.5% min, Al=0.4%, Ti=0.4%, Ni=32.5% | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 7.94*10³ | kg/m³ | 496 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 196 | GPa | 28500 | ksi | 
| Thermal expansion (20 ºC) | 14.4*10-6 | ºCˉ¹ | 8.0*10-6 | in/(in* ºF) | 
| Specific heat capacity | 460 | J/(kg*K) | 0.11 | BTU/(lb*ºF) | 
| Thermal conductivity | 11.5 | W/(m*K) | 80 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 98.9*10-8 | Ohm*m | 98.9*10-6 | Ohm*cm | 
| Tensile strength (annealed) | 600 | MPa | 87000 | psi | 
| Yield strength (annealed) | 275 | MPa | 39900 | psi | 
| Elongation (annealed) | 45 | % | 45 | % | 
| Liquidus temperature | 1385 | ºC | 2525 | ºF | 
| Solidus temperature | 1357 | ºC | 2475 | ºF | 