| Non-heat-treatable Nickel-Chromium-Iron Alloy Inconel 600 | ||||
| Chemical composition: Cr=15.5%, Fe=2.5%, Ni=72% min. | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.47 *10³ | kg/m³ | 529 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 207 | GPa | 30000 | ksi |
| Thermal expansion (20 ºC) | 13.3*10-6 | ºCˉ¹ | 7.4*10-6 | in/(in* ºF) |
| Specific heat capacity | 444 | J/(kg*K) | 0.106 | BTU/(lb*ºF) |
| Thermal conductivity | 14.9 | W/(m*K) | 103 | BTU*in/(hr*ft²*ºF) |
| Electric resistivity | 103*10-8 | Ohm*m | 103*10-6 | Ohm*cm |
| Tensile strength (annealed) | 655 | MPa | 95000 | psi |
| Yield strength (annealed) | 310 | MPa | 45000 | psi |
| Elongation (annealed) | 45 | % | 45 | % |
| Liquidus temperature | 1354 | ºC | 2470 | ºF |
| Solidus temperature | 1350 | ºC | 2460 | ºF |