| AISI 316 | ||||
| Chemical composition: C=0.08%max, Mn=2%max, Cr=17%, Ni=12%, Mo=2.5% | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.0 *10³ | kg/m³ | 499 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 193 | GPa | 28000 | ksi | 
| Thermal expansion (20 ºC) | 15.9*10-6 | ºCˉ¹ | 8.8*10-6 | in/(in* ºF) | 
| Specific heat capacity | 502 | J/(kg*K) | 0.12 | BTU/(lb*ºF) | 
| Thermal conductivity | 16.2 | W/(m*K) | 112 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 7.4*10-7 | Ohm*m | 7.4*10-5 | Ohm*cm | 
| Tensile strength (annealed) | 586 | MPa | 85000 | psi | 
| Yield strength (annealed) | 241 | MPa | 35000 | psi | 
| Elongation (annealed) | 55 | % | 55 | % | 
| Hardness (annealed) | 80 | RB | 80 | RB | 
| Tensile strength (cold drawn) | 620 | MPa | 89900 | psi | 
| Yield strength (cold drawn) | 415 | MPa | 60200 | psi | 
| Elongation (cold drawn) | 45 | % | 45 | % | 
| Hardness (cold drawn) | 91 | RB | 91 | RB | 