| Cast copper alloy C90300 (Tin Bronze) | ||||
| Chemical composition: Sn=8.3%, Zn=4.0%, Cu=87.5% | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.80 *10³ | kg/m³ | 549 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 96.5 | GPa | 14000 | ksi | 
| Thermal expansion (20 ºC) | 18.0*10-6 | ºCˉ¹ | 10.0*10-6 | in/(in* ºF) | 
| Specific heat capacity | 377 | J/(kg*K) | 0.090 | BTU/(lb*ºF) | 
| Thermal conductivity | 74.8 | W/(m*K) | 518 | BTU*in/(hr*ft²*ºF) | 
| Electric resistivity | 14.5*10-8 | Ohm*m | 14.5*10-6 | Ohm*cm | 
| Tensile strength (sand cast) | 310 | MPa | 45000 | psi | 
| Yield strength (sand cast) | 145 | MPa | 21000 | psi | 
| Elongation (sand cast) | 30 | % | 30 | % | 
| Hardness (sand cast) | 70 | HB(500) | 70 | HB(500) | 
| Liquidus temperature | 1000 | ºC | 1832 | ºF | 
| Solidus temperature | 854 | ºC | 1570 | ºF | 